How Do You Cure Plastisol Ink With a Conveyor Dryer?

Home › Ask Buckets › Cure plastisol with a conveyor dryer

BI
Buckets of InkSpecs from published maker data · Tempe, AZ
Short answer

Plastisol cures when the total thickness of the ink layer reaches 320 to 340 F, according to Vastex. A conveyor dryer carries the printed shirt under infrared heat for a consistent time, and you control cure with the belt speed (time) and heater temperature.

Vastex dryer ratings at a 25 second cure

DryerPlastisol shirts/hr
D-100110+
D-100-WL110+
D-1000110+
LittleRed X2-30260+
LittleRed X2-54520+
LittleRed X3-30360+
LittleRed X3-54720+
EconoRed II-30300+

Steps

  1. Print the shirt and place it on the dryer belt.
  2. Set the belt speed and heater temperature so the whole ink layer reaches 320 to 340 F.
  3. Check the cure on the first shirts, then run production.
  4. Use an exhaust hood to remove fumes at the exit.

Why ratings differ

Vastex bases shirts-per-hour estimates on 16 in centers; ink maker and shop humidity change the result. Water-based and discharge inks are rated at 70 seconds. See the dryer finder.

Frequently asked questions

What temperature cures plastisol?

Vastex: the whole thickness of the ink layer must reach 320 to 340 F.

How long should plastisol stay in the dryer?

Vastex's ratings use a 25 second cure for plastisol; follow your ink maker's cure data too.

Related: Dryer finder

Have a question for our shop? Call or text 480-229-7806 (Monday to Friday, 7:30 AM to 4:00 PM Arizona time) or send us a message. Want to see a machine run? Visit our demo room in Tempe, AZ during the same hours. In-stock orders placed by 2:30 PM Arizona time ship the same day from Tempe, AZ. Need equipment? Get a quote.We Bring the Store to Your Door.